Skill v1.0.0
currentAutomated scan100/100name: cold-spraying description: Cold spray coating — kinetic energy deposition, critical velocity, bonding mechanism, powder materials (Cu/Ti/Al/MCrAlY), coating properties, process parameters, HVAF comparison, SAE AMS2440. metadata: version: "1.0.0" priority: 7 promptSignals: phrases:
- "cold spray"
- "cold spraying"
- "kinetic spray"
- "cold gas dynamic spray"
- "cold spray coating"
minScore: 3
Cold Spray Coating — Complete Skill
Process Fundamentals
Cold spray: supersonic particles (300–1200 m/s) impact substrate at solid state (no melting) → bonding through adiabatic shear instability and plastic deformation Temperature: particles < melting point; typically 100–600°C gas temperature (vs. 2000–3500°C for thermal spray) Pressure: 20–70 bar driving gas (N₂ or He)
No oxidation: particles bond without melting → minimal oxide formation Compressive residual stress: particle impact → compressive stress (unlike tensile in APS) No phase transformation: feedstock retained (WC, cermets, reactive metals)
Critical Velocity
Critical particle velocity for bonding: v_crit = √[4σ_f (1 + C_p T_p / (σ_f/ρ))] / √ρ [m/s; simplified]
Empirical model (Assadi et al.): v_crit = -0.25 (T_m - T_i) + 667/(ρ_p) - 14 (σ_UTS/ρ) + 0.08 T_m + 7 c_p
Practical critical velocities:
| Material | v_crit [m/s] | |
|---|---|---|
| Copper | 570–600 | |
| Aluminum | 680–720 | |
| Titanium | 700–900 | |
| Steel | 550–650 | |
| MCrAlY | 750–850 | |
| Ni | 620–650 |
Above v_crit: adiabatic shear at particle-substrate interface → intimate bonding Below v_crit: particles bounce off (erosion of substrate); no coating builds
Particle velocity from nozzle: v_p = v_gas × [1 - exp(-π c_D ρ_gas r_nozzle² L / (4 m_p))] [approximate] Or: use isentropic flow + drag equations; typically v_p = 0.85–0.95 × v_gas
Gas velocity (converging-diverging nozzle): At exit: v_gas = M_exit × a_exit [M = exit Mach from nozzle design; a = sound speed at T_exit]
Gas Selection
Nitrogen (N₂): Lower molecular weight (28 vs. He 4) → lower particle velocity P = 20–70 bar; T = 300–800°C Lower cost; most common for Cu, Al, Ni v_gas ≈ 500–700 m/s at nozzle exit
Helium (He): 4× higher sound speed → much higher particle velocity v_gas ≈ 1200–1500 m/s; much higher v_p possible Use for: high-strength alloys requiring high v_crit (Ti, steel, ceramics); expensive (~10× N₂) Often He at 5–15 bar gives same v_p as N₂ at 70 bar
Powder Materials and Properties
Copper (Cu)
Applications: electrical conductivity (additive repair, bus bar, electronics); corrosion barrier Process: N₂ at 30 bar, 500°C; v_p = 600–800 m/s; easily exceeds v_crit Coating properties: Porosity: < 0.5%; electrical conductivity: 85–90% IACS Hardness: 120–150 HV (work-hardened vs. 70–80 HV annealed Cu) Thermal conductivity: 340–380 W/(m·K)
Titanium (Ti, CP Ti)
Applications: aircraft repair, corrosion protection, bone implant coating Process: He or high-P N₂; T = 600–700°C; v_p = 800–1000 m/s Properties: Porosity: 1–3% (N₂ spray); < 0.5% (He spray) Oxygen content: 0.5–0.9% (vs. 0.15% for wrought; some oxidation even without melting) Adhesion: > 50 MPa (cold spray); requires bonding temperature
Aluminum (Al)
Applications: aircraft structure repair, galvanic protection, thermal management Process: N₂ at 25–40 bar, 300–500°C Properties: Porosity: 0.5–2% Electrical conductivity: 30–40 MS/m (vs. 37 MS/m for wrought) Adhesion: 40–70 MPa
MCrAlY (Bond Coat Alternative)
Cold spray MCrAlY: preserves chemistry; no Y₂O₃ oxidation (critical for TBC adhesion) Process: He + high P; T = 700–900°C gas T Properties: Lower oxidation than HVOF MCrAlY → better TBC life Porosity 1–3%; densification by HIP improves properties
Process Parameters
| Parameter | Effect | |
|---|---|---|
| Gas pressure ↑ | v_p ↑ → better bonding; less porosity | |
| Gas temperature ↑ | v_gas ↑ (sound speed ↑); material softer → lower v_crit | |
| He vs. N₂ | He: much higher v_p; much higher cost | |
| Particle size ↓ | v_p ↑; too small → poor inertia; optimal 10–45 μm | |
| Stand-off distance | Optimal typically 15–40 mm | |
| Spray angle | Best at 90°; < 45° → porosity increases significantly |
Deposition efficiency (DE): DE = mass deposited / mass fed × 100% [typically 50–80% above v_crit; strongly material-dependent]
Comparison to HVAF/HVOF
| Feature | Cold spray | HVOF | HVAF | |
|---|---|---|---|---|
| Temperature | Below melting | Near-melting | Very low | |
| Oxidation | Minimal | Moderate | Low | |
| Phase preservation | Excellent | Good | Excellent | |
| Velocity | 300–1200 m/s | 600–900 m/s | > 900 m/s | |
| Residual stress | Compressive | Compressive | Compressive | |
| Porosity | < 0.5–3% | 0.5–2% | 0.5–2% | |
| Best for | Reactive metals, thick deposits, repair | WC-Co, MCrAlY | WC-Co |
Standards
| Standard | Scope | |
|---|---|---|
| SAE AMS2440 | Cold spray metallic coatings | |
| ASTM B532 | Porosity measurement for coatings | |
| AMS2449 | HVOF (for comparison; cold spray being added) | |
| MIL-STD-1687 | Thermal spray coatings (being updated for cold spray) |
Output
Provide: powder material and size [μm], driving gas (N₂/He) and pressure [bar], gas temperature [°C], nozzle type (de Laval), estimated particle velocity v_p [m/s] vs. v_crit [m/s], coating thickness [μm] per pass and total, porosity [%], hardness [HV], adhesion strength [MPa], residual stress (compressive), deposition efficiency [%], application (repair/protection/additive), and applicable standard (SAE AMS2440).